12 years 10 months ago #1168 by Archived Forum Admin
H/C wire breakage photos was created by Archived Forum Admin
Hello All,
Sometimes we have wire breakages during roping and we could not find the reasons why ? do uou have any breakages photos related breakages which shape results for patenting, high reduction, or wire rod?
best regards.
Murat
Murat
Sometimes we have wire breakages during roping and we could not find the reasons why ? do uou have any breakages photos related breakages which shape results for patenting, high reduction, or wire rod?
best regards.
Murat
Murat
Please Log in to join the conversation.
- Archived Forum Admin
- Topic Author
- Offline
- Platnium Boarder
12 years 10 months ago #1169 by Archived Forum Admin
Replied by Archived Forum Admin on topic Re: H/C wire breakage photos
To stop breakages during stranding high carbon steel wires:
1.- Do not over stress the wire during drawing, try to use a small total reduction of area to allow the wire to be able to stand further work during stranding. Meet tensile by carbon content.Check torsion to meet specifications.
2.- Check the patenting in order to obtain full austenization of the wire and right structure by correct time and temperature on the austenization furnace and the cooling furnace.
3.- Check the design of the cable to be sure it has the right lay
4.- Check strander to be sure all guides are in good shape.
For patentig structures can be seen in the wire Handbook of WAI in the patenting section.
Regards
Eduardo Anaya
Senior Consultant
INDEPA S.C.
Mexico City
Tel(011-52)555-407-7451
This email address is being protected from spambots. You need JavaScript enabled to view it.
1.- Do not over stress the wire during drawing, try to use a small total reduction of area to allow the wire to be able to stand further work during stranding. Meet tensile by carbon content.Check torsion to meet specifications.
2.- Check the patenting in order to obtain full austenization of the wire and right structure by correct time and temperature on the austenization furnace and the cooling furnace.
3.- Check the design of the cable to be sure it has the right lay
4.- Check strander to be sure all guides are in good shape.
For patentig structures can be seen in the wire Handbook of WAI in the patenting section.
Regards
Eduardo Anaya
Senior Consultant
INDEPA S.C.
Mexico City
Tel(011-52)555-407-7451
This email address is being protected from spambots. You need JavaScript enabled to view it.